Typical Physical Properties of Compounds of ADIPRENE
ADIPRENE TYPE
|
L42 |
L100 |
L167 |
L315 |
Hardness, Durometer Value
(ASTM d676-59T) |
80A |
90A |
95A |
75D* |
| Specific Gravity |
1.07 |
1.10 |
1.13 |
1.21 |
|
Tensile Strength, MPa (psi)
(ASTM D412-61T)
|
20.7 (3,000) |
31.0 (4,500) |
34.5 (5,000) |
62.0(9,000) |
|
Elongation At Break, %
(ASTM D412-61T)
|
800 |
450 |
400 |
270
|
|
100% Modulus, MPa (psi)
(ASTM D412-61T)
|
2.8 (400) |
7.6(1,100) |
12.4(1,800) |
32.0(4,650) |
|
Compression Set, %
Method B (ASTM D395)
Method A (ASTM D395)**
|
45
-
|
27
9 |
40
10 |
-
10 |
|
Resilience, %
Rebound (Bashore)
|
- |
45 |
40 |
45 |
|
Impact Resistance,
Izod notched
J/m (ft.lb./In)
(ASTM D256)
+24 Degrees C (+75Degrees F)
-40 Degrees C (-40 Degrees F)
|
Flexed
- |
Flexed
- |
Flexed
- |
800.7(15)
58.7 (1.1)
|
|
Solenoid Brittle Temp.,
Degrees C (Degrees F)
(ASTM D746-57)
|
Below -80 (Below -120) |
Below -70 (Below-94) |
Below -70) (Below -94) |
-64
(-83) |
|
Abrasion Index, NBS, %
(ASTM D1630, Nat'l Bureau of Standards Abrader)
|
110 |
175 |
400 |
435 |
|
Tear Strength Split, kN/m (pli)
(ASTM D470)
|
12.2(70) |
13.1 (75) |
26.2 (150) |
192.2 (110) |
|
* The D Scale is used to measure durometer hardness above 95A by
Shore, Rex, or Wallace durometers.